Limiting Draw Ratio by Material: DC04, 304 and 5052
Limiting draw ratio (LDR) is the largest blank-diameter to punch-diameter ratio a single draw can survive without tearing. The values we quote from our own presses are DC04 2.1–2.2, 304 stainless steel 1.85–2.05 and 5052 aluminum 1.80–1.95. A lower LDR does not mean an inferior material; it means the same shell needs one more reduction, and possibly an anneal between them.
Key point: LDR converts a material choice into a stage count: DC04 takes the biggest first reduction, 304 stainless steel needs more stages because it work-hardens, and 5052 aluminum needs the most.
What LDR actually measures
In a cylindrical draw the blank is held at the flange while the punch pulls material radially inward over the die radius. The tensile load in the cup wall rises with blank diameter; past a limit the wall tears at the punch nose. The ratio of the largest successful blank diameter to punch diameter is the LDR, a standard formability index described in the deep drawing process and in ASM Handbook Volume 14B. Sheet formability itself is characterised by ASTM E517 (plastic strain ratio) and ASTM E646 (strain-hardening exponent).
LDR is a press-and-tool figure, not a material constant found in a handbook. Blank holder force, die radius, lubrication and sheet temper all move it, which is why we publish the bands measured on our own 5–500 ton presses rather than a single ideal number. The full limiting draw ratio chart shows the bands together; the calculator applies them to a blank diameter.
Reading the three bands
DC04, 2.1–2.2. A low-carbon deep-drawing steel with high uniform elongation. It takes the largest first reduction and is the default when corrosion resistance is not required.
304 stainless steel, 1.85–2.05. Austenitic stainless steel work-hardens rapidly and springs back after the punch releases, so stages are shallower and an intermediate anneal may be needed before the final sizing pass. Sheet certification follows ASTM A240/A240M; the reasons are set out in material selection for deep drawing.
5052 aluminum, 1.80–1.95. The most formable of the common aluminium grades we draw, but still below steel. A tall seamless can therefore needs more reductions than the same geometry in DC04. 6061 is not on this list: we do not deep draw 6xxx sheet, as explained in Can 6061 Aluminium Be Deep Drawn?.
From ratio to stage plan
Once the first reduction is fixed, the remaining depth is gained by redraws; ironing thins the wall without changing diameter. Formed dimensions hold ±0.05 mm, tightening to ±0.02 mm after ironing, and our capacity page states those bands once. Draw depth is quoted to 150 mm, tooling is built in-house, minimum order is 1,000 pieces and a quote returns within 24 hours. Inspection records follow ISO 9001.
Decision table
| material | LDR band | consequence for the stage plan |
|---|---|---|
| DC04 low-carbon steel | 2.1-2.2 | Largest first reduction; fewest stages |
| 304 stainless steel | 1.85-2.05 | Shallower stages; work hardening may require an anneal |
| 5052 aluminum | 1.80-1.95 | One more reduction than the same shell in DC04 |
| 6061 aluminum T6 | Not drawn | Cracks on a deep draw; shallow forming only |
| Any grade, non-round shell | LDR applies less directly | Corner radius governs material flow |
Frequently asked questions
Is LDR a fixed property of the material?
No. It is the outcome of a specific press, tool and lubrication setup. The r-value and n-value measured by ASTM E517 and ASTM E646 describe the sheet, but the LDR we quote is the band we have actually formed on our own presses.
Why does 304 stainless steel have a lower LDR than DC04?
Austenitic stainless steel work-hardens rapidly as it deforms and springs back after the punch releases, so the wall loses ductility sooner. Reductions are shallower and an intermediate anneal may be needed before a final sizing pass.
Can 5052 aluminum match a DC04 shell without extra stages?
Rarely. With an LDR of 1.80-1.95 against 2.1-2.2 for DC04, the same depth-to-diameter geometry normally needs one more reduction. The trade-off is weight and corrosion behaviour, not forming speed.
How do I use LDR to estimate the number of draws?
Divide the required blank diameter by the punch diameter to get the drawing ratio, then compare it with the band for the chosen grade. If the ratio exceeds the band, plan a redraw; repeat until the final diameter and depth are reached. The calculator does this arithmetic for you.
Does ironing change the limiting draw ratio?
Ironing is a separate pass that thins and straightens the wall; it does not increase the first-draw LDR. It does let you hold +/-0.02 mm on the wall and bore, which is why it appears after, not instead of, the draw schedule.
Do you publish an LDR for 6061 aluminum?
No. We have not measured one on our presses and we do not deep draw 6xxx sheet, so publishing a value would imply a capability we do not offer. 6061 is used for shallow forming, with heat treatment afterwards if the print requires T6 strength.
What we do not claim: We do not publish leak-rate figures, autoclave cycle counts, springback angles or furnace recipes that we have not measured on our own parts. The ±0.02 mm figure applies to ironing passes only, not to every geometry. 6xxx aluminium is used for shallow forming, not deep drawing. Prices, minimum order quantities and lead times are confirmed per drawing rather than published as fixed values.
Last reviewed: 2026-11-05 · Reviewed by Sam Zhang, Process Engineer. See the full Deep Drawing Engineering Guides hub for process comparisons, measured draw ratios and defect troubleshooting.