Can 6061 Aluminium Be Deep Drawn?

Deep Drawn Aluminum Battery Housing

6061 aluminium can only be deep drawn in its soft annealed O temper, and even then it is the wrong alloy for the job. In T6 condition it cracks on a deep draw. At AUNOV we do not deep draw 6xxx sheet: we use it for shallow forming and, when the print calls for final strength, heat treat to T6 after the part is shaped. For a genuine deep drawn shell we specify a 5xxx alloy instead — 5052 aluminium is the one we measure and quote against.

Key point: The answer depends on temper, not just alloy name. “6061” on a drawing is not a complete material specification; “6061-T6” is a hard, high-strength condition that will not survive a deep draw, while “6061-O” is soft enough to form but still loses to 5052 on draw ratio, consistency and cost.

Why the temper decides the answer

6061 is a heat-treatable Al-Mg-Si alloy. Its mechanical properties come from precipitation hardening, so the same chemistry behaves completely differently before and after heat treatment. The 6061 aluminum alloy reference lists the common tempers: O (annealed, softest, most ductile), T4 (solution treated and naturally aged) and T6 (solution treated and artificially aged, the strongest and most widely stocked).

What buyers usually mean by “6061” is 6061-T6 sheet from a stockist. That material has roughly five times the yield strength of the annealed condition and far less elongation. Put it over a draw punch and the flange cannot feed; the wall thins at the punch radius and splits. This is not a lubrication problem and a bigger die radius will not fix it. The plastic strain ratio r, defined in ASTM E517, and the strain-hardening exponent n, defined in ASTM E646, are the two sheet properties that predict whether a blank will flow or tear — and T6 scores badly on both.

6061-O is a different material in practice. Annealed sheet is soft, has high elongation and can be formed into shallow shells and complex bends. The usual industrial route is to form in O or T4 condition, then solution treat and age up to T6 afterwards. That route is real, but it adds a heat-treatment step, brings distortion and quench risk on thin walls, and still does not give you the drawability of a non-heat-treatable forming alloy. Tool geometry and forming limits for this family are covered in ASM Handbook, Volume 14B.

What we use instead, and the numbers behind it

The limiting draw ratio (LDR) is the largest blank diameter a sheet can be pulled into a given punch diameter in one operation before the bottom tears out. We measure it on our own presses rather than quoting a handbook value. Our working figures:

Material Measured LDR Deep draw route
DC04 low-carbon steel2.1–2.2Single deep draw; the reference material
304 stainless steel1.85–2.05Deep draw with controlled blank-holder force
5052 aluminium1.80–1.95Deep draw; our default for aluminium shells
6061-T6 aluminiumNot drawn by usShallow forming or machining only
6061-O aluminiumNot publishedShallow forming; T6 after forming if required

5052 is a non-heat-treatable Al-Mg alloy built for forming. The 5052 aluminium alloy reference describes it as a medium-strength sheet alloy with good workability and corrosion resistance — which is exactly the combination a drawn can, cover or sensor shell needs. Our measured LDR for 5052 is 1.80–1.95, high enough for a real multi-stage draw without an intermediate anneal on most geometries. Full method and the rest of the table are on our limiting draw ratio chart.

Tip: If a drawing says only “aluminium 6061” with no temper, ask what the part actually needs. Nine times out of ten the requirement is corrosion resistance and low weight, not T6 yield strength — and 5052 will give you a sounder shell at a lower tooling risk.

Where the process limits sit

These are the envelopes we hold on drawn work, and they apply whichever alloy is chosen: press lines from 5 to 500 tons, draw depth up to 150 mm, general tolerance ±0.05 mm and ±0.02 mm where an ironing pass is added. Ironing and redraw are not interchangeable; the ironing vs redraw guide explains what each pass does to the wall. The ±0.02 mm figure applies to ironing only, not to every geometry.

For a shallow, stiff, machined-from-solid part, 6061-T6 remains a good choice — we machine it in our own CNC cells every week. The mistake is specifying it for a seamless deep shell. If the part needs a sealed, one-piece wall, compare drawn vs machined vs welded housings before you fix the material; the forming route and the machining route solve different problems. Our material selection for deep drawing guide covers the full grade trade-off, and deep drawing vs metal spinning covers the case where volume is too low for a draw die.

What we do not claim

We do not publish a limiting draw ratio for 6061 because we have not measured one on our presses. We do not publish leak rates, autoclave cycle counts or springback angles for any alloy. We do not list prices, SKUs or customer reviews on product pages. The figures in the table above are measured on our own tooling for the grades we actually draw; they are not a general guarantee for every coil lot or every geometry. If your print calls for 6061 and a deep shell, we will tell you at quotation stage rather than discover it at tryout.

How to specify it on the drawing

Give the alloy, the temper and the functional requirement separately. “5052-H32, deep drawn, wall continuity required” is a specification a die shop can work to. “6061” alone is not. If final strength genuinely requires a 6xxx alloy, say so and we will quote the forming-plus-heat-treatment route, or a machined alternative, with the distortion risk written into the process plan. Quotes are returned within 24 hours, tooling is made in-house, and the minimum order quantity for new tooling is 1,000 pcs. See our product families for the shapes this applies to.

FAQ

Can 6061-T6 aluminium be deep drawn without cracking?

No. T6 is solution treated and artificially aged, which raises yield strength and cuts elongation to the point where a deep draw tears at the punch radius. Form in the annealed O temper first, then heat treat to T6 afterwards if the print requires that strength. Expect to manage distortion on thin walls.

Why is 5052 aluminium our default instead of 6061 for drawn shells?

Because 5052 is a non-heat-treatable forming alloy with a measured limiting draw ratio of 1.80 to 1.95, and it keeps that ductility through the whole draw without a post-form heat treatment. 6061 only becomes formable in the annealed condition and then needs solution treatment and ageing to reach the strength people specified it for. DC04 low-carbon steel and 304 stainless steel draw to higher ratios when weight is not the constraint.

Why is 6061-O not used for production deep drawing?

It can be formed, but the route needs an annealed blank plus a solution treatment and age after forming, which adds distortion risk and cost on a thin wall. A 5xxx forming alloy reaches the same shape without that step. We use 6xxx sheet for shallow forming and machining, not for seamless deep shells.

Does heat treating 6061 to T6 after forming change dimensional tolerance?

It can. Quenching a thin 6061 shell moves dimensions, so a tolerance that was held at the press is not necessarily held after solution treatment and ageing. We quote to the final condition: general tolerance ±0.05 mm on drawn work, ±0.02 mm only where an ironing pass is part of the route. Features tighter than that are machined after heat treatment, and the print should state the tolerance at the final temper rather than at the formed blank.

At what draw depth does a 6061 shell need a multi-stage route?

Depth alone does not decide that; the blank-to-punch draw ratio does. Our presses cover draw depths up to 150 mm across a 5 to 500 ton range. Once the ratio exceeds the measured limit for the grade, the route is split into stages with an intermediate anneal only where the metal demands it. For 6xxx sheet we do not plan a deep multi-stage draw at all — we plan shallow forming or a different alloy.

What should I do if my drawing specifies 6061 for a sealed can?

Ask whether T6 strength is functionally required. If it is not, 5052 gives a sounder seamless wall. If it is, the realistic routes are shallow forming followed by heat treatment, or machining from solid, both of which we quote with the distortion and tolerance consequences stated up front. Send the drawing and we will come back within 24 hours.

Technical review: Sam Zhang, Process Engineer. See the full Deep Drawing Engineering Guides hub for process comparisons, measured draw ratios and defect troubleshooting.

Last reviewed: 2026-11-05 · Reviewed by Sam Zhang, Process Engineer