What Is the Maximum Draw Depth for a Deep Drawn Part?
The deepest draw we quote as a published capability is 150 mm. Depth is not an isolated limit: it is the product of blank diameter, material, wall behaviour and the number of reductions the part can survive. A 150 mm deep round can in DC04 is a different job from a 150 mm square enclosure, because the corners of a non-round shell see different material flow at every angle.
Key point: 150 mm is our published draw-depth ceiling; beyond that we quote after a drawing review, and the real constraint is usually the depth-to-diameter ratio rather than the millimetre figure.
Where the 150 mm figure comes from
Deep drawing is defined by plastic flow: a flat blank is pulled over a punch radius into a die while a blank holder controls the flange, as described in the standard process description and in the DIN 8584 classification of forming by drawing. The deeper the shell, the more reductions are needed, and each reduction consumes ductility. Our press range of 5–500 ton and our tool shop set the mechanical envelope; the 150 mm figure is the depth we will quote against that envelope without a special review.
Stage planning starts with the limiting draw ratio. DC04 reaches 2.1–2.2, 304 stainless steel 1.85–2.05 and 5052 aluminum 1.80–1.95. Those bands are laid out in the LDR chart and converted to a stage count by the drawing calculator. A part needing three reductions is still within the 150 mm range if the material and the tool layout agree.
When depth forces a different plan
Two passes change different things. A redraw pulls an already-drawn cup through a smaller die to reduce diameter and gain depth; ironing squeezes the wall through a gap narrower than the sheet thickness to thin and straighten it. The distinction is set out in Ironing vs Redraw. When accumulated cold work leaves too little ductility for the next reduction, an intermediate anneal restores it — the mechanism is recrystallisation, covered in ASM Handbook Volume 14B.
Non-round geometry is the other common reason a deep part is harder than its nominal depth suggests. Square and rectangular shells wrinkle at corners while the opposite wall tears, so corner radius and stage count are decided before the press is chosen. Formed dimensions hold ±0.05 mm as standard and ±0.02 mm with ironing; ISO 9001 governs the inspection records behind those figures.
How we quote a part beyond the published range
Send the drawing with the finished diameter, depth, wall, material and the dimensions that carry a functional tolerance. Formability data such as the strain-hardening exponent (ASTM E646) helps us judge how far the grade can be reduced. We return a stage plan and a quote within 24 hours, with tooling built in-house and a minimum order of 1,000 pieces per part number. Where a very deep seamless shell would need more reductions than the material can take, we say so and propose an alternative route rather than promising a depth we cannot hold. The drawn vs machined vs welded comparison explains when a fabricated or machined route is the honest answer.
Decision table
| part requirement | what governs the answer | where to check |
|---|---|---|
| Round shell up to 150 mm | Depth-to-diameter ratio and LDR | Limiting draw ratio chart |
| Beyond 150 mm | Drawing review before quoting | Send the print for a stage plan |
| Deep and narrow | Redraw stages and ironing | Ironing vs Redraw |
| Deep and square/rectangular | Corner radius and uneven material flow | Irregular deep drawn parts |
| Deep with work-hardening grade | Intermediate anneal between stages | Material selection guide |
Frequently asked questions
Is 150 mm a hard limit on every geometry?
It is our published capability, not a universal physical limit. A round can in a formable steel grade reaches it more easily than a square enclosure of the same depth. Above 150 mm we review the drawing and issue a stage plan rather than declining on the millimetre figure alone.
Does a deeper part always need more press tonnage?
Not automatically. Tonnage follows blank diameter, material strength and drawing force; depth mainly adds reductions. Our 5-500 ton range covers both a small deep cup and a large shallow cover, so press size and stage count are separate decisions.
Does a conventional draw thin the gauge, or only an ironing pass?
In conventional drawing the wall is not deliberately thinned; it is the ironing pass that reduces gauge and straightens the wall. We hold +/-0.05 mm on formed dimensions and +/-0.02 mm after ironing, and we state which features receive that pass on the quote.
Can a single draw produce a 150 mm deep shell?
Only for a favourable blank-diameter-to-punch-diameter ratio. The limiting draw ratio of the grade caps the first reduction; DC04 reaches 2.1-2.2, 304 stainless steel 1.85-2.05 and 5052 aluminum 1.80-1.95. Anything beyond that needs redraws.
What is the risk of pushing depth without an intermediate anneal?
Work hardening raises yield strength and consumes ductility, so the next reduction tears at the punch radius. An anneal between stages restores ductility by recrystallisation. We do not publish a furnace recipe; that belongs on the heat-treatment specification.
Which dimensions should be toleranced on a very deep shell?
Only the features that matter functionally, typically the bore, the sealing face and the overall height. Over-tolerancing a deep shell adds sizing or machining passes without improving fit. Our quote separates formed dimensions from finished ones.
What we do not claim: We do not publish leak-rate figures, autoclave cycle counts, springback angles or furnace recipes that we have not measured on our own parts. The ±0.02 mm figure applies to ironing passes only, not to every geometry. 6xxx aluminium is used for shallow forming, not deep drawing. Prices, minimum order quantities and lead times are confirmed per drawing rather than published as fixed values.
Last reviewed: 2026-11-05 · Reviewed by Sam Zhang, Process Engineer. See the full Deep Drawing Engineering Guides hub for process comparisons, measured draw ratios and defect troubleshooting.