Oxygen Sensor Cup – Drawing Ratio

Oxygen sensor cup
Oxygen sensor cup

The cup is where the drawing ratio is decided

Of all the parts in a gas sensor, the oxygen sensor cup is the one that most directly determines whether the geometry is manufacturable. A cup is a closed-end cylinder – the sensing element’s protective shell, the reference-air chamber, or the outer shield depending on the sensor architecture. It is drawn from flat strip, and the single number that governs the whole process is the draw ratio: the blank diameter divided by the cup diameter.

For a first draw we keep the ratio at or below 1.8-2.0 for austenitic stainless steel, and below 1.6 for the ferritic grades used at very high temperature. Exceed those and the wall thins past the point where the cup tolerates thermal cycling; the base tears or the side wall necks. Cups that need a ratio above 2.0 are drawn in two operations with an inter-anneal or at least a stress-relief between passes.

Wall thickness distribution – the number nobody specifies and everybody needs

A drawn cup is never uniform. The base stays close to the blank thickness while the wall thins toward the open end; the thinning is governed by die clearance and by how the material flows over the punch nose. For a sensor cup we typically see 8-15% thinning at the mid-wall and up to 20% at the open rim if the process is pushed. Two consequences follow:

  • The base must carry the blank thickness for the weld or the element seat. We design the first draw so the base retains at least 92% of nominal, then redraw only the wall if a deeper cup is required.
  • The rim must survive a crimp or a weld. A rim thinned to 0.7 mm from a 1.0 mm nominal will crush unevenly; we keep rim thickness within 10% of nominal by increasing the die radius and reducing blank-holder force.

We verify distribution by sectioning three cups per lot and measuring seven points from base centre to rim, not by a single micrometer reading.

Geometry envelope and tooling route

  • Cup diameter: 8-45 mm typical for sensor bodies; up to 60 mm for large diesel sensors.
  • Depth: up to 3.5× diameter with a two-stroke process, 1.5× in a single stroke.
  • Thickness: 0.4-1.2 mm.
  • Base features: flat, dimpled, or pierced for a reference-air port – each adds one station to the die.

Because sensor cups are high-volume (millions per year in automotive), the tooling is almost always a progressive die running from coil. The die combines blanking, draw, redraw where needed, trim, and any piercing in one strip, so cycle time stays in the tens of milliseconds and per-piece cost is dominated by material, not by machine time.

Exhaust-side corrosion: what the cup sees

An outer cup faces exhaust condensate – a cocktail of nitric and sulfuric acid at 100-600 °C, plus road salt spray from outside. Material choice and surface condition decide the life:

1.4301 (304)Standard choice, adequate for most gasoline applications in mild climates.
1.4404 (316L)Preferred where condensate is aggressive or the sensor sits close-coupled; molybdenum content resists chloride pitting.
1.4512 / 1.4509Ferritic, for high-temperature thermal-fatigue resistance; lower corrosion margin, so not for road-salt-exposed outer shields.
Aluminised steelCost-driven option for non-critical inner shields; not for the gas-facing cup.

A passivation step after forming removes free iron and drawing-lubricant residue from the surface; skipping it is a common cause of early red rust on a cup that should have lasted the vehicle life.

Forming defects to watch

The three defects that most often reject a sensor cup lot:

  1. Earing – a scalloped rim caused by planar anisotropy in rolled strip. We control it by specifying texture-controlled material and by trimming the rim after the draw rather than relying on a net blank.
  2. Orange peel / surface roughening – appears when a coarse grain structure is stretched heavily. A finer ASTM grain size (7 or finer) keeps the surface smooth through the draw.
  3. Base fracture from a tight punch radius – the punch nose radius for stainless steel should not fall below 2t; below that, fracture is a matter of time even if the first article passes.

Heat treatment between draws

When a cup needs two draws, the work hardening from the first pass must be addressed. For thin walls we often skip a full anneal and use a controlled redraw that exploits the residual ductility, but for ratios beyond 2.2-2.4 an inter-anneal in a bright, hydrogen atmosphere is required. That anneal is also where the material recovers the corrosion resistance that cold work degrades, so we treat it as a corrosion step as much as a forming step.

Wall thickness is a distribution, not a dimension

Can you hold 0.02 mm on the wall thickness? No – wall thickness is a distribution, not a dimension. We hold the base and rim thicknesses within band and give you a sectioned report showing the profile, which is what actually matters for strength and sealing.

How deep can a single cup go? About 1.5× diameter in one stroke. Beyond that we either redraw or, for very deep reference chambers, switch to a tube-based route that we supply through our partner lines.

Do you pierce the reference-air port in-die? Yes, when volume justifies it. In-die piercing keeps the port concentric to the bore within 0.1 mm and avoids a second fixture.

What drives the price? Material grade first, then annual volume (which amortises the progressive die), then the number of secondary features. A cup with a pierced base and a coined rim costs more than a plain cup at the same diameter.

Specifying a cup for quoting

Give us the cup diameter, depth, wall thickness, base feature, material grade, and annual volume. If the ratio is above 2.0 and you need a single-piece part, tell us early – that decision changes the tooling route, the inter-anneal, and the lead time, and catching it at the quotation stage is far cheaper than catching it on the first production lot.

This part sits inside our Sensor Housings range. Across the sensor housings pages you will find the process notes, common materials and inspection points behind every product in the family.

Specifications

ItemOxygen sensor cup
BrandAUNOV
DesigningYour drawing sets the part – samples are reverse-measured into a controlled drawing; changes are priced before they are made.
ToolingDies, fixtures and gauges are made in our own toolroom, so the die charge appears as its own quotation line, and the die remains dedicated to your part.
SamplesFirst-article samples ship with a dimensional report and material certificate, so any deviation is corrected at sample stage, and later batches are gauged back to the signed sample.
MaterialsStock covers carbon steel (SPCC / DC01), 304 / 316 stainless steel, aluminium and brass; mill certificates and heat numbers accompany the first article.
Surface finishSurface treatment matched to the duty: plating, coating or polishing; the agreed finish travels with the part number.
ProcessingDeep drawing first, CNC finishing on critical faces after; first articles check the complete flow before we release the run.
EquipmentHydraulic presses for drawing, with CNC turning for finishing, with in-house toolmaking to keep dies and fixtures maintained.
Tolerance+/-0.01 mm on sealing faces, +/-0.05 mm on drawn profiles; GD&T per drawing, PPAP-style reports on request.
Delivery termsCIF or DDP, with FOB available, T/T or L/C, with D/P accepted on repeat business; each volume tier carries its own quoted price.

Frequently Asked Questions

Why is the cup the part that decides whether the whole sensor geometry is buildable?

Because it carries the deepest reduction. Of all the drawn pieces in the assembly, the cup asks the most of the material in the fewest operations, so its draw ratio sets what every other stage has to accommodate. Once that ratio is settled the remaining geometry tends to fall into place, and until it is, none of the neighbouring parts can be costed honestly.

Everybody needs wall distribution and nobody specifies it – why?

Because it is not one number. A drawn cup thins unevenly, and what matters is where the minimum falls relative to where stress and corrosion are worst. A nominal wall hides the possibility that the thinnest place and the most vulnerable place coincide, so the useful call-out is a minimum wall in a stated location rather than a wall thickness generally.

What does the exhaust side actually attack on this cup?

Condensate rather than hot gas. Exhaust condensate is aggressive, it collects where the part runs coolest, and it works preferentially on the regions already thinned by drawing. Selecting material against gas temperature alone leaves that mechanism untouched, which is why the corrosion requirement belongs on a separate line from the temperature requirement.

Why does heat treatment appear between draws rather than after them?

Because drawing removes ductility progressively, and once it is gone the material will not survive the next reduction. Annealing between stages restores enough formability to continue, at the cost of a furnace pass and a cleaning step. That is why the stage plan includes heat treatment from the outset instead of having it added after a draw has already gone wrong.

Request a Quote for This Part

Send a drawing or sketch — get material advice, tooling cost and a per-piece price within 24 hours (working days).